Page 117 - The Effect of Hydrogen and Hydrides - ebook first test
P. 117

    (40)       (45)     (40)
                                                                      = 40       (45)
                                                                         






























                  Figure 4-47:   Correlations between fractions of radial hydride formation and hoop stress for: (a) hydride number and (b) hydride
                             lengths for different Zircaloy-2 cladding, all having Zr liners and for different HRTs (from [Aomi et al., 2009]).

























                  Figure 4-48:   Effect of cooling rate of HRT on (a) radial hydride orientation in terms of ratios, Fl(45) and Fn(40), and (b) sum of the
                             lengths of all hydrides and only radial hydrides. Results are for Zircaloy-2 cladding with Zr liner used in BWRs (from
                             [Aomi et al., 2009]).





                                                                                           
                                     (40)       (45)
                                                                




                                                                 (40)      (45)




                                   Copyright © Advanced Nuclear Technology International Europe AB, ANT International, 2019.