Page 125 - The Effect of Hydrogen and Hydrides - ebook first test
P. 125
Figure 4-56: Temperature dependence for BWR Zircaloy-2 cladding with liner for HRTs at different applied hoop stress values and
a cooling rate of 30C/h (0.5°C/min). The experimentally determined hydride reorientation ratios have been adjusted to
account only for dissolved hydrogen as contributing to hydride precipitation (from [Aomi et al., 2009]).
≥
⁄
log (40) 1
≥
≅
= 400℃ < 400℃
< 400℃
,
⁄
log (40) 1 1/
log (40) log (40) 1 1/
⁄
(40) (40)
1
(40) =
1 + 49 ∙ [− ∙ ]
3
(∆ )
Copyright © Advanced Nuclear Technology International Europe AB, ANT International, 2019.